Development without toxic TMAH – the new choline developer from Allresist

October 2026

TMAH is an established developer for photoresists and electron beam resists. Due to its high toxicity, we are looking for alternatives that enable high-performance processes while reducing potential hazards. Choline hydroxide is a promising option: free of metal ions, readily biodegradable and delivering impressive development results. In addition, choline hydroxide has substantially lower oral toxicity than TMAH.

In collaboration with Fraunhofer ENAS in Chemnitz, we obtained excellent results in development trials with the electron beam resist Medusa 84 SiH. Compared with TMAH (AR 300-73), 45% choline hydroxide maintained high sensitivity and achieved a slightly higher contrast of γ = 4.3. Choline hydroxide thus demonstrated the highest technological precision in developing this HSQ resist, with negligible health risk.

Fig. 1 Contrast curves for Medusa 84 SiH at different choline hydroxide concentrations

Fig. 2 80 nm dots written at a dose of 520 µC/cm² (50 kV)

Trials with various photoresists showed that using choline hydroxide as an alternative to TMAH does not necessarily compromise process performance. For novolac-based photoresists, the development rate can be matched to that of 2.38% TMAH by selecting a suitable concentration. For the resists investigated, the corresponding choline hydroxide concentration was found to be approximately 4.3–4.35%. The experimental data are shown in Figure 3. Choline hydrochloride at 4.3% is therefore a direct substitute for TMAH and can be used as a drop-in replacement in existing development processes.

Figure 3: Experimental investigation of the dissolution rates of slow- and fast-dissolving novolacs as a function of choline hydroxide concentration. Comparison with 2.38% TMAH shows equivalent dissolution rates at concentrations of 4.3–4.35%.

Choline hydroxide developers from Allresist

Allresist offers choline hydroxide-based developers under the product names AR 300-41 (45%) and AR 300-42 (4.3%). They provide a TMAH-free development option for various photoresist and HSQ processes. The appropriate concentration depends on the resist and the specific process conditions.

Choline hydroxide combines a more favourable toxicological profile with high-performance development, expanding the options for more responsible process chemistry. This is why we have selected this developer as our “Resist” of the Month.